Steel Flattening Test

 Jun 18, 2021

 Leave a message

 

Requirements for flattening test specimens for steel pipe


The steel pipe samples for the flattening test should be cut from the steel pipes that have passed the visual inspection. The length of the steel pipe test sample should not be less than 10mm, but not more than 100mm. The length of the sample is chosen to be 40mm when doing the experiment. The edges of the steel pipe test specimens are allowed to be rounded or chamfered. When cutting the sample, it is necessary to prevent damage to the surface of the sample, or to change the properties of the steel pipe due to heating or cold process.


Steps of the flattening test


1.When performing a flattening test, the test sample should be placed between two parallel flat plates, as shown in figure a.

2. For the flattening test, uniform pressure should be applied to the end of the specimen or steel tube of the specified length , until the distance between the two pressure plates reaches the value specified in the product standard. Test should under load, as shown in Figure b.

3. In the case of close flattening, the contact width of the inner surface of the sample is at least 1/2 of the width of the sample after flattening, as shown in Figure c.

4. When flattening test for welding steel pipes, the position of the weld should be specified in the relevant standards. If not specified, the weld should be located at a position 90°.

5.The test is usually carried out at room temperature, and the moving speed of the platen when the sample is flattened should not exceed 25mm/min.

6. The length of the pressing plate should exceed the width of the sample after flattening, that is, at least 1.6 times the outer diameter of the tube. The width of the pressure plate should not be less than the length of the sample. The pressure plate should have sufficient rigidity.

7. After the steel pipe test sample is flattened to the specified distance, remove the load and remove the sample. Evaluate the test results in accordance with the requirements of the relevant steel pipe product testing standards. If no specific requirements are specified, no visible cracks on the sample after the flattening test shall be assessed as qualified. Only slight cracks at the edges of the sample shall not be considered as scrap.


Attention in flattening test

1. If the steel pipe test sample is marked on the surface, when the flattening test is performed, the marked surface of the sample should be in contact with the lower surface of the pressure plate, and it should not be placed at the angle of 90°with the applied force.


2 After the flattening test is over, remove the upper and lower pressure plates.



Send Inquiry